In This Article
Have drawings to evaluate? Upload them for a quote
Direct Answer
Zhongde Precision has anodized the following aluminum parts for power equipment.
| Part | Main purpose | What to agree in advance |
|---|---|---|
| Heatsinks and fins | Corrosion protection, appearance, heat dissipation | Contact face masking, trapped solution, film thickness |
| Aluminum housings and enclosures | Corrosion protection, appearance, insulation, wear | Grounding point masking, color by material, rack mark position |
That job covered anodizing only, on parts supplied by the customer. Under our confidentiality agreements, we do not publish customer names, drawings or part photos. This article only describes the part types and what we watched during finishing.
1. Scope of the Work
We handled the surface finishing step only, not machining or assembly. When finishing supplied parts, scratches, dents, porosity and oil left by earlier steps can become more visible after anodizing. It is important to check the parts on arrival and agree with the customer how defects that existed before finishing will be handled.
Zhongde Precision handles CNC machining, anodizing and assembly in house. Doing machining and finishing together makes it easier to adjust machining conditions for the needs of the finish.
2. What Power Equipment Parts Need from Anodizing
For heatsinks and housings in power equipment, anodizing is usually expected to do several jobs:
- Corrosion protection: limits corrosion of aluminum in outdoor cabinets or humid installations.
- Appearance: gives exterior parts a consistent color and texture.
- Insulation: anodic film does not conduct electricity and is sometimes used for surface insulation.
- Heat dissipation: black anodizing has high emissivity and helps natural-convection heatsinks shed heat by radiation.
- Wear resistance: reduces scratches during handling.
The same non-conductive film on a heat transfer face can be a problem for some parts. That is why masking, covered next, matters.
3. Masking Grounding Points and Thermal Contact Faces
3.1 Grounding and Conductive Faces
Grounding terminal seats, faces where bolts connect housings electrically, and mating faces that need shielding cannot conduct through the film. These areas are masked or have the film removed after finishing. Please mark which faces must be conductive, with their extent, on the drawing.
3.2 Thermal Contact Faces
Faces in contact with power devices, modules or thermal pads depend on heat transfer and flatness. Whether to keep the film, mask the face or machine it after finishing depends on the thermal design and insulation approach, so we follow the customer design intent.
3.3 Masking Boundaries
Masking uses plugs, tape or masking compounds depending on the area. The boundary leaves a small step in the film, so if a boundary falls on a visible face, its position and acceptable appearance should be agreed.
4. Heatsink and Fin Geometry
Deep, narrow fins exchange solution poorly, and film thickness tends to differ between fin tips and roots. Solution trapped between fins can leave white marks or stains after drying. Racking orientation, solution exchange, rinsing and drying conditions are set to suit the geometry.
Thorough sealing keeps the corrosion resistance and color of the film stable.
5. How Material and Earlier Steps Affect the Result
Anodizing results depend heavily on the material and on earlier process steps.
| Material or earlier step | Effect on anodizing |
|---|---|
| Extrusions (such as 6063) | Film tends to be uniform; common for heatsinks |
| Machined wrought parts (such as 6061) | Stable results; tool marks and extrusion die lines still show |
| Die castings (such as ADC12) | High silicon; film tends to be gray; porosity and color variation show |
| Mixed materials | Colors differ even under the same conditions |
If one product combines extruded heatsinks with die-cast housings, matching the color is difficult, so decide first how much difference is acceptable. Causes and control of color variation are covered in controlling anodizing color variation, and cosmetic anodizing of die castings in high-cosmetic anodizing of die-cast aluminum.
6. Dimensional Change
Anodic film grows both into and out from the base metal, so threaded holes, fitted bores and assembly datums change with film thickness. Where this matters, those areas are masked or machining dimensions are set with the finished dimension in mind. The approach is explained in dimension control before and after anodizing.
7. Rack Marks and Appearance Standards
Anodizing connects each part to an electrode, so the rack contact point always leaves a mark. We agree the contact positions with the customer so rack marks stay off visible faces.
Appearance judged by words alone drifts easily. Agreeing color and acceptable marks and unevenness with limit samples keeps judgments consistent from lot to lot.
8. How This Relates to PCS and Power Module Cooling Parts
Cooling parts and housings for PCS, inverters and IGBT and SiC power modules raise the same questions:
- Which faces are grounded and which are insulated
- Flatness and heat transfer on faces in contact with power devices
- Corrosion protection in outdoor energy storage systems
- Appearance differences when extrusions, machined parts and die castings are combined
Liquid cold plates and manifolds are covered in manufacturing IGBT and SiC power module cold plates and on our liquid cooling parts page.
9. What to Send When Requesting a Quote
New projects can start with samples. Send us the following, and we will confirm the finishing conditions before quoting.
| Item | Details |
|---|---|
| Drawings | Part drawings with masked areas, conductive faces and contact faces marked |
| Material | Alloy grade (extrusion, machined part or die casting) |
| Film | Film type, color, sealing |
| Appearance | Visible faces, acceptable rack marks and unevenness, limit samples |
| Quantity | Sample quantity and expected production volume |
| Supplied parts | Condition on arrival, handling of defects present before finishing |
| Packaging | Protection for fins and visible faces, cleanliness requirements |
Frequently Asked Questions
What did Zhongde Precision do on the power equipment parts?
We anodized aluminum heatsinks and fins and aluminum housings and enclosures supplied by the customer. The job covered surface finishing only, with no machining. Under our confidentiality agreements, we do not publish customer names, drawings or part photos.
Are there areas on power equipment parts that should not be anodized?
Anodic film does not conduct electricity, so grounding terminal seats and faces that rely on bolts for electrical contact must be masked or have the film removed after finishing. Faces in contact with power devices or thermal pads may also be masked, depending on heat transfer and flatness requirements. These areas should be specified on the drawing.
Can die-cast housings be anodized?
Yes, but high-silicon die-cast alloys tend to give a gray film, and color variation and porosity can be visible. Matching the color of extruded or machined parts is difficult, so the appearance standard and limit samples should be agreed in advance.
Does anodizing change dimensions?
Yes. The film grows both into and out from the base metal, which affects threaded holes, fitted bores and assembly faces. Where this matters, those areas are masked or machining dimensions are set with the finished dimension in mind.
Can machining and anodizing be ordered together?
Yes. Zhongde Precision handles CNC machining, anodizing and assembly in house. Ordering them together lets us set machining conditions with the dimensions and appearance after anodizing in mind. Please tell us the material, quantity, film type and color, masked areas and appearance standard.